Lecture 34 : WPCBs recycling: Hydrometallurgical processes

IIT Kanpur July 201
20 followers
2 Video Views·Oct 4, 2024
Greetings, I welcome you all to the new lecture for this course, and we have been discussing
till now the methods of recycling electronic waste, wherein we have been discussing some
general electronic wastes. And our main focus was on waste printed circuit boards, and we
have discussed the delamination and the pyrometallurgical route of recycling the WPCBs. Now, in this
lecture we will be sort of concluding our investigation, and we will be discussing the
pyrometallurgical route of recycling WPCBs. And here we will be emphasizing on what are
the general important aspects that one must take care of while designing a holistic route
of recycling WPCBs, and what are the challenges that people have faced.
Some of the important laboratory investigations will also be highlighted in the end, and gradually
we will be then moving towards the next aspect of electronic waste, which will be focused
on the battery recycling. So, coming back to the hydrometallurgical route of WPCBs,
we know that in pyrometallurgical route we have the pyrolysis, and the different processes
that are involved in pyrometallurgy. They have their own advantages, they these processes
can lead to the generation of pyrolysis products, apart from what we get as the mixture which
can be further processed to get the metals. So, we know that there are different advantages
of pyrometallurgical processes, but at the same time when we are looking at regeneration
of hazardous gases that can cause health hazards. We think about hydrometallurgy which does
not have these hazardous implications. So, we will begin on that hydrometallurgical recycling
of WPCBs, and we know that similar to pyrometallurgy we already have the hydrometallurgical route,
and we have discussed it for metallurgical waste as well. So, the same concept will be
applied for the WPCB for recovery of valuable materials. So, basically recovery of valuable
materials, but here in actually we are supposed to ask a couple of questions, what are so
the questions are what are these valuable materials that can be extracted. So, a probable
answer could be we have metals, base metals, precious metals and of course, hazardous metals.
We do not wish to use hazardous metals, but we need to extract this to keep the whole
environment safe, then we have refractories, refractory oxides and polymers. So, these
are the valuable materials that can be extracted. The next question could be what are the appropriate
procedure steps involved in this process. So, a generalized outline can be made. So,
we need retreatment, which is again appropriate suitable for hydrometallurgy. Then we need
the leaching of reagents, leaching with reagents again choice of reagent is a good thing to
consider. Then we need to purify purification of reagents of in this case it will be leach
it will be recovery of valuables from liquor and residue and then of course, it will finally,
we will have development of products. Now, retreatment followed by leaching followed
by purification and then we get the development of products. So, this is the appropriate procedure
that we can think of when we are having a generalized outline of WPCB recycling, which
appears pretty much similar to any other hydrometallurgical route that we have been discussing. So, and
it means that in general the outlines remains the same. It is just that we are going to
change the raw feed, we are going to change. Similarly, we are going to change the reagent
the operation parameters might change the recovery that we might get for various reagents
and operation parameters are going to change. And then we should be gradually optimizing
them to get the best fit and then further recovery can be done using the leach liquor.
So, the same will be followed for WPCBs. Now, what are the key parameters? The next question
could be what are the key parameters that basically govern the efficiency of the process.
What are the key parameters of the process? So, we know that for hydrometallurgical processes
there are there is the choice of reagent, we have temperature range, duration which
is basically time, time of reaction. We have solid liquid ratio, pH of solution, pH of
solution, feed size, particle size, agitation at times it is very important. And if we are
looking at bio leaching we might also need aeration and so many other parameters that
are important for bio leaching and the such leaching operations which basically use the
microorganisms. So, these are the key parameters that are involved in optimizing the overall
efficiency of the process. Now, we are now going to discuss specific
processes that are involved for WPCBs. So, we know that WPCBs are basically a set of
processes which can be subjected to disassembly or dismantling. And then we can go for damaged
PCs and WPCBs and if we have let us say usable PCs we separate them out. And we know that
we have what we are actually trying to do here is basically mechanical and chemical
processes. We know the different types of pretreatments that are generally used for
these operations and then we also know that we are going for separation. After separation
we are having the metal fraction and the non metal fraction which can be further processed
as in hydrometallurgical route or pyrometallurgical route. So, we are assuming that it has followed
a path line starting from WPCB collection to disassembly to damaged EC for further separation
and then going into the separation of the metal fraction and the non metal fraction.
And then another classification between hydrometallurgy and pyrometallurgy. So, now we are going to
discuss hydrometallurgical route assuming all of these processes are already done.
Another important aspect that we should be considering before we jump here is importance
of EC removal before hydrometallurgy. Why? Why should we focus specifically on EC removal?
This is very important because it interferes with the hydrometallurgical process. What
are the reasons? So, there is a risk of or chance of explosion.
During reaction this is possible if we are if the EC somehow react with the reagent itself
or the risk of chance of generation of hazardous chemicals or it can also lead to the various
hydrocarbons which can be very much hazardous to the humans. Generation of hazardous chemicals
this will be formed due to leaching of epoxy resins or any other hydrocarbon that is present.
And then the third one excessive use of reagent excessive use and of course, unwanted use
of reagent for leaching because it is going to get partitioned. So, suppose I have some
leaching reagent it will be partitioned into various end results and the leaching efficiency
that we expect will not be achieved because it is getting consumed by various PRs or hydrocarbons
etcetera. So, this is something that we do not wish to entertain what we wish is we should
be using the leaching reagents for leaching purposes only. So, this splitting of or excessive
consumption of reagents for unnecessary reaction and that to that reaction is going to render
our leach leaker hazardous. So, it should not be encouraged what we can
do is just remove the ECs directly go for the WPCB leaching and this is how we should
be approaching our raw material. Now, there are some important ways by which we can remove
these ECs by hydro metallurgical route as well. So, one can think of use of KBR as a
reagent that is possible people have tried using it for metal recovery and it has given
some good results. The other option could be if we have let us say solder alloy. So,
where is solder alloy? Solder alloy will be attached to the soldering joints where we
have attached our ECs. So, if we wish to approach the solder alloy recovery then we can and
we wish to do it through hydro metallurgy then such reagents can be opted for.
Now, right now we are assuming that the ECs are already removed, but in case if we wish
to remove it through hydro metallurgy then it becomes an alternative. This process becomes
an alternative to the conventional desoldering process. So, solder alloy leaching has been
projected and this can be done by using methanosulphonic acid and what we can do is we can remove the
can be done along with methanosulphonic acid is we can have additions of H 2 O 2 as well.
This really helps in the solder alloy leaching. Now, we will directly jump into the important
flows of WPCBs. So, we have let us say WPCBs and right now I am assuming that important
pretreatment has been done as discussed here. So, after that we have primary leaching one
can have let us say H 2 S O 4 plus H 2 O 2. This is just an example we can have so many
numerous examples coming in here in as a choice for primary leaching and then we can have
decoppered material because this can actually lead to copper recovery. This is just an example
and then we can go for using decoppered materials we can go for let us say H N O 3 leaching
which is basically the second stage leaching. If this is primary stage leaching we can have
a secondary stage leaching here. The second stage leaching which can give us let us say
silver recovery and this can again give us let us say if it has gold then gold residue
if at all it is there and then this can be further processed for gold leaching and recovery.
This could be the last stage. So, again it depends upon what type of metal are we targeting
here in this in this very simple flow sheet we have assumed three elements copper is the
waste metal gold and silver are precious metals. This the complexity increases when we are
having numerous metals in the picture and we know that in reality WPCBs have numerous
elements with varying concentrations and the sample tends to change which means the complexity
of the problem is very high and one has to design how we are going to extract the base
metals how we are going to extract the precious metals what are the elements that we can extract
first or later. So, that really governs our choice that what
is the reagent that we will be using as our primary leaching reagent then our secondary
leaching reagent or if there is a third stage leaching then what should be using in what
should be used in the third stage. So, it depends on the complexity of the process and
what is the final target of the whole recovery procedure. Similarly, we can have a different
route. So, if we have processed WPCBs again we are assuming that some pretreatment procedure
has been done and along with PCPs we have ICs. So, again complete of WPCBs considered
which is been pretreated then we can have let us say leaching with reagents you can
have adsorption wherein we can add let us say activated carbon because we are thinking
of adsorption. So, we need to have some means for some material that we need to use for
adsorption. So, let us say activated carbon is that material and then this can give us
gold recovery after adsorption we process it to get gold or at the same time since we
are using this we can have ion exchange we can perform elution and then this can also
give us gold. So, we have gold recovery by precipitation or cementation. So, this means
we have so many different routes by which we can recover our materials and in this case
we have just focused on gold and right now we are assuming that we are able to recover
our base metals as well. Now, thinking on gold recovery from WPCBs
gold recovery is usually performed by using cyanides cyanide leaching is one of the common
routes and this applies for WPCB as well. So, leaching with reagent one of the most
common reagent would be cyanides if we do not wish to go into cyanides. So, non cyanide
reagents include there are non cyanide reagents. So, thiosulphates thiourea halogenates and
so on so forth. So, these also have good recoveries of course, the leaching parameter changes.
So, one should really mind whichever process we are trying to follow leaching parameters
vary with the reagent and of course, there is the addition of H 2 O 2 and F e 3 plus
F e 2 S O 4 whole thrice to basically improve the leaching in case of let us say thiosulphates
thiourea. So, basically all additions can be done to improve the process, but again
it is just dependent upon what reagent we are trying to really use.
Now, we are going to discuss some of the most important findings that people have described
in their work and how it really impacts the whole leaching procedure. So, let us first
look at the leaching procedure. So, it will these tables are going to help us understand
how the leaching procedure is done and we already know that the recovery after leach
liquor is going to be either through ion exchange solvent extraction precipitation or electro
winning or cementation. So, different routes are already available with us the most crucial
step actually is the first step itself how we are conducting our leaching experiments.
So, we will discuss on this and we will make these tables and these are this table is specially
for the base metal. So, we will write base metal recovery and we have leaching reagent
conditions and then recovery. So, if we are using H 2 S O 4 just as an example we have
added this. So, we have let us say 20 m l H 2 S O 4 plus 20 m l H 2 O 2 we can get let
us say 99.4 percent copper. Similarly, 85 degree Celsius 12 hours 2 molar H 2 S O 4
we get 100 percent copper and zinc 68 degree Celsius 4 hours 1.6 molar H 2 S O 4 we can
have let us say 98.2 percent copper. Then let us say we have 50 degree Celsius 2 molar
H 2 S O 4 and H 2 O 2 addition. So, we can have 46 percent copper and 51 percent zinc
we have let us say H N O 3 this was for H 2 S O 4. Now, if we write for H N O 3 we have
let us say 6 molar H N O 3 15 minutes reaction duration 6 15 minutes to let us say 6 hours
and 80 degree Celsius we see we can reach nearly up to 100 percent copper 2 to 5 molar
H 2 S O 4 H N O 3 70 degree Celsius 2 hours 99 percent copper 3 molar H N O 3 60 degree
Celsius again 5 hours 50 percent copper 93 percent zinc.
This tells us that a wide variety of recoveries can be described let me just quickly highlight
of information and we see that copper is just getting recovered very quickly just by using
very common reagents. What happens if we are going to go ahead and switch our reagent for
a different metal all together? What happens if we are going for bio leaching? And we see
that H 2 S O 4 and H N O 3 are good reagents the one just has to think about increasing
time at times or increasing molar concentration or at times one can think of increasing S
by L ratio or agitation this might help. When we look at the case of precious metals
we will have we will have again the same leaching reagent operations what are the operation
conditions recovery. So, in this case let us say we have N A C N sodium cyanide we see
that 4 grams per liter sodium cyanide is taken for 15 days this can give us let us say gold
of 46 percent silver 51 percent. So, if now we are taking thio urea then we
can say let us say 20 grams per liter this thio urea is taken and I have mentioned we
need to add let us say Fe 3 plus ions or some other additions and let us say 0.5 molars
H 2 S O 4 this type of addition is at times important to help us increase our overall
metal recovery. So, suppose that 121.1 milligrams per liter of silver is recovered and this
could be having 24 grams per liter and then we use room temperature also. So, this can
give us 90 percent silver 90 percent gold finally, thiosulphate. So, in this case it
is ammonium thiosulphate ammonium thiosulphate. So, if this is the case then we have 0.1 molar
ammonium thiosulphate in this case we are going to use 40 millimoles of C O S O 4 10
grams per liter per density which is basically S by L and this case we need 8 hours and they
mentioned R P M also. So, 250 R P M and this gives us 56 percent gold mentioning some of
precious metal. So, this is precious metal recovery the last
one that we are supposed to discuss is basically bio leaching. So, bio leaching because it
is a one of the most important advancing technology that people have been exploring
for material recovery. In this case we are using microorganisms and then bio leaching
conditions and then recovery a ferro oxidants ferro oxidants. So, we have let us say in
this case one has to actually mention as much as possible what is the size this is the size
of the WPCB actually 93 micrometer pH is 2 17 to 20 days because one has to keep it for
very long period 80 percent copper recovery. Similarly, if you have 1.78 to 2.2 50 millimeter
size pH again is 2.25 they kept it for 183 hours and Fe 3 Fe 2 plus addition is let us
say 9 grams per liter you get 92 percent copper. And if let us say if we have a different microorganisms
we have acidophilum a acidophilum then we can have 60 m l a acidophilum supernatant.
So, this is basically supernatant and then we have 15 m l H 2 O 2 60 degree Celsius kept
for 2.5 hours this can give us nearly 100 percent copper again putting up some references
here. So, we have so in the all these 3 tables that we have seen this one is for bio leaching
the previous one was for precious metal and the one before that was for base metal.
We see that there are different types of parameters that people have described in their research
and different overall recoveries. Now, we know that these parameters can vary depending
on reagents and the raw feed that they have the values may not appear to be very much
consistent the reason behind that itself is because the PCV compositions are not consistent.
We have already emphasized that e waste is a waste that can vary from sample to sample
from source to source. So, the recoveries can change and people have been exploring
wide variety of reagents for their overall recovery. I will like to mention 2 important
strategies for final recoveries that people have explored one is polymer inclusion membrane
and the other is the organic solvent displacement precipitation strategy. So, when we think
of organic solvent utilization it helps us in precipitating out the solvents solutes
that are present in the aqueous medium and polymer inclusion membranes are those membranes
that can help us in isolating the specific metal ions from the leach liquor. These are
really new strategies that have been utilized for metal recovery from WPCVs and other complex
leach liquors that have been explored. Till now we have covered extensively the delamination
the pyrometallurgy and the hydrometallurgy. In the upcoming classes we will be discussing
about the e waste the next segment of e waste which will be basically on the recycling of
batteries. Thank you.