Step inside a working 20th-century brickyard and follow the complete process of traditional brick making — from raw clay in the pit to finished, fired brick. In this Aged Skills history episode, filmed in 1988 near Meckenheim, Germany, we document the full production cycle at a surviving Meckenheim Ring Kiln — one of the last operational Hoffmann-style ring kilns still working in regular service. The film begins at the clay face, where a bucket-wheel excavator cuts two centimetres at a pass, carefully controlling groundwater to maintain the right consistency for pressing. From there, side-tipping mine cars haul the clay to the press building, where rollers, an edge runner mill, and a de-airing auger press transform it into a continuous clay column. A fully automatic wire cutter slices the column into green bricks at a rate of up to 2,500 per hour. We observe how moisture is balanced by experience rather than automation — monitored through motor load, vacuum pressure, and the operator’s trained eye. Green bricks dry for up to two weeks in open sheds before being hand-set inside a 1907 oval ring kiln.
Inside the kiln: • 14 chambers fire in a continuous cycle • The main fire travels counter-clockwise over 8–14 days • Temperatures reach 1,080°C in the peak firing zone • Lignite slack fuel is dropped through timed feed hoppers • Residual heat pre-warms incoming loads
Before walls can rise, clay must be won and dried.
In today's Age Skills History episode, we travel to 1988, to a clay works near Meckenheim in Germany.
Here, clay is cut from the pit, pressed and wire cut into green bricks, dried in open sheds,
and set by hand inside a ring kiln that burns day and night.
A bucket wheel excavator works steadily along a cut face roughly 60 to 70 metres long.
Each bucket strips away just 2 centimetres of clay at a pass, breaking the material up in the process.
The operator keeps the bucket row pressed hard against the base of the face,
taking up as little ground water as possible.
Clay that is too wet causes problems at the press and wire cutter,
and the same goes for clay that is too dry.
The excavated clay drops through a chute into side-tipping mine cars,
each holding around three quarters of a cubic metre.
Four cars coupled together make up a single train.
A simple mechanical linkage keeps each car tracking alongside the sideways travelling excavator.
A small diesel locomotive then hauls the four loaded cars back to the press building.
In the background, a settling pond is visible, dug out from an exhausted section of the clay pit
and now put to use by the syrup factory.
Since there has been no rain for several days, the clay is running dry.
Water will need to be added during pressing to bring it back to the right consistency.
Once the locomotive driver uncouples the four cars, he hooks the first onto a cable winch.
A ramp hoist carries it up to the charging floor above the press.
The Meckenheim ring kiln has a rated capacity of one and a half to two million bricks per year.
In 1988, with demand on the lower side, around 600,000 bricks will be fired.
At full output, the press can produce approximately 26,000 green bricks per day, known in the trade as cakes.
A floor-mounted hook holds the car steady while it tips.
The clay falls directly into the feed hopper below, which is approximately four metres long and holds nearly five cubic metres.
The empty car is then lowered back down the ramp hoist and returned to the clay pit.
A conveyor carries the clay through a pair of rollers and into the edge runner mill,
where heavy grinding wheels break it down and force it through a screen.
The two grinding wheels are connected to the line shaft via a flat belt and clutch.
Up on the charging floor, the hopper attendant has already worked some water into the dry clay to loosen it up and improve workability.
The ground clay falls onto a slowly turning pan, where a rotating auger pushes it through an opening onto the feed belt running into the brick press.
That belt runs at a steady speed, though the press operator can adjust the feed rate up or down as the job demands.
Inside the press, a heavy auger continues breaking down and blending the clay while pushing it forward into the de-airing chamber.
The first formed product to emerge is the extruded clay column, fed out continuously through the die.
The column rides along a belt to a fully automatic wire cutter, which slices it into individual green bricks.
The entire press is driven by a set of V-belts. The motor and belts keep turning even when the press is thrown out of gear.
The heart of the press is the de-airing chamber, where a vacuum pump draws the air out of the clay,
a step that prevents cracking during both drying and firing.
It runs at a negative pressure of 0.8 to 0.9 bar, with an external gauge confirming the seal is holding.
When the clay is too wet, it blocks the de-airing chamber and stops production.
The press operator throws the press out of gear and shuts down the edge runner mill.
The chamber is opened and the clay fouling the glass inspection port and interior walls is scraped away.
Only once the chamber is cleaned out and resealed can the vacuum be properly restored,
so the press operator works through it carefully before closing up again.
With the press back online, the operator keeps a steady watch on the emerging clay column.
His most useful instrument is the ammeter, which reflects the motor load and gives an indirect reading of the clay's consistency.
If the clay is too soft or too wet, the current drops below the normal mark of 110 amperes.
To head off another blocked chamber, the operator feeds a few dried green bricks, known as blanks, back through the edge runner mill.
They grind down and pull the surplus moisture out of the mix.
If the clay runs too dry, water is added into the hopper or directly into the press.
The column now comes through the die cleanly and evenly,
though faint transverse lines are still just visible, a trace of the clay having been slightly too wet.
The automatic wire cutter runs at a rate of 1.5 seconds per cut,
around 2,500 green bricks per hour, or 20,000 per shift, assuming steady running.
Actual output on the day of filming comes to around 18,000.
Two parallel pairs of setting boards carry 12 green bricks apiece,
which are then repositioned with the two end bricks squared off.
The hoist rack holds two pairs of setting boards per shelf, 24 green bricks in all.
Across ten shelves, the total capacity comes to 240 green bricks.
When the rack is full, the bricks are transferred using the trolley frame.
The trolley carries the green bricks to one of two drying sheds,
which together hold between 320,000 and 330,000 green bricks.
In fair weather, around 14 days is enough for the bricks to dry out to firing condition.
The drying racks are laid out to let the wind move freely between the boards and around each brick,
with the gaps between bricks sized accordingly.
Meanwhile, the kiln master is already bringing in fuel,
a reminder that shaping and firing run in parallel throughout the working day.
Freshly pressed and cut green bricks have a dark, glossy surface.
As they dry, they become paler and more matte.
Once the fresh bricks have been unloaded into the drying shed,
the trolley goes back out carrying a load of already dried green bricks,
from here on called blanks, bound for the setting area beside the kiln.
When the trolley frame is pulled clear of the board pairs,
the hoist rack automatically closes down to a tighter pitch,
matching the hand truck used to carry 120 blanks to the ring kiln.
Since setting is moving at a good pace today,
the driver picks up a second frame carrying 240 blanks,
while a worker heads for the kiln with the hand truck already loaded.
The frame is pivot mounted so that the board pairs, blanks and all, can be turned lengthwise.
Only in that orientation do they clear the 90 cm wide chamber doors of the ring kiln.
Ring kilns came into general use from the 1860s onward,
replacing the slow, fuel-hungry clamp firings that had served brickmakers for centuries.
The ability to fire without ever letting the kiln go cold was a genuine step forward,
and the fuel savings gave it a strong commercial case as well.
The Meckenheim kiln was built in 1907.
The original drawings survive, showing the floor plan, kiln layout,
side elevation and several cross sections.
The kiln measures approximately 35 m long and 12 m wide.
The crown stands 3 m and 40 cm above the floor,
and the outer circumference runs to around 86 m.
Fourteen chambers are arranged in a continuous oval around the central chimney stack,
each closed off by a door during firing.
The fire travels counter-clockwise around the oval,
completing a full circuit in eight days at normal pace,
or up to 14 days when firing slowly.
At any given time, blanks are being loaded into two chambers,
while finished bricks are being drawn from the others.
In the remaining chambers, the charge is preheating, firing and cooling in turn.
Each chamber is 4 m and 80 cm long and 2 m and 50 cm high.
Above each chamber run four or five rows of feed holes,
three per row, through which fuel is dropped onto the ware below.
A single horizontal layer of blanks inside the chamber is called a course.
The course sitting directly beneath the feed holes is the fire course.
Because of how the courses are stacked,
fuel dropped from above falls through the feed holes all the way to the kiln floor.
Following the spacing of the feed holes, every fourth course is set as a fire course.
Each chamber takes 16 courses of 500 blanks each.
Right now, the main fire is working through two and a half chambers,
spanning 40 to 45 courses.
Twelve rows of automatic feed hoppers are in position above the main fire chambers.
A mechanical timer trips them at regular intervals,
dropping measured charges of fuel through the feed holes.
Combustion air enters through the two open chamber doors at the cool end,
sweeping forward past the already fired ware and into the main fire.
The exhaust gases draw away through the 52-metre chimney stack.
Active work in the kiln takes place roughly two chambers ahead of the main fire.
The first gang, working with the kiln master, is loading blanks into the chamber.
A second gang is busy pulling finished bricks out on the far side.
In the chambers beyond, the fired bricks are cooling down.
Two chambers are currently running on residual fire,
a lighter burn that follows once the main fire has moved through.
Across the six rows of the residual fire zone,
temperatures ease from 1,020 degrees down to around 900 degrees.
As the main fire advances, the residual fire moves with it.
We now follow the loading and firing sequence in close detail.
The individual courses have been stacked high enough
that a paper damper can be hung across the chamber opening.
Cut from waxed paper, it stops the draft from pulling in the wrong direction,
and you can see clearly how the drawer presses it flat against the front course.
The flues directly behind the damper are left open,
so the waste heat pre-warms the incoming blanks.
Every operation in the kiln has to mesh with the others.
The loading gang depends on a steady supply of blanks from outside
to hold their piecework rate.
For this documentary, the two kiln masters demonstrate the old stacking method.
In what is known as diagonal setting, blanks are stood at an angle, head to head.
The open arrangement lets the fire circulate more freely,
but the angled blank presses a shallow impression into the face of the brick beneath it,
a mark that is still easy to spot today in the exposed brickwork of older buildings.
The four-course plinth, however, is the same in both old and new methods.
The kiln masters now lay the next course,
taking particular care with the lowest layer of the plinth.
Blanks are set on as level a surface as the kiln floor allows,
so the finished stack sits true and does not lean.
This modern approach is called the packed setting.
The kiln floor is littered with ash and clinker baked hard from earlier firing cycles.
About five to seven centimetres of this build-up has to be cleared away every three to four years.
Here the kiln master positions a full feed hole,
meaning the right-hand section of the fire course falls directly beneath the opening above.
That is not always straightforward, since the holes do not always line up in a neat row.
Getting the blanks set correctly takes real experience,
and it makes a direct difference at the firing stage.
Kiln masters have a saying for it – well set is half fired.
Because of the kiln's curved walls, the centre feed hole does not sit directly over its opening.
The kiln master compensates by shifting a half-width feed position forward by one step.
In the next course he mirrors it, shifting a half-width position back,
so the two halves together form one complete feed shaft.
The fire course is done.
On the right, the full feed hole is correctly positioned.
The centre one is still offset forward.
While stacking continues in the base chamber, the kiln master turns to closing the chamber door.
The first leaf is two bricks thick, 24 centimetres, and is built tight against the inner kiln wall.
The same bricks are reused each time, stacked ready on the outside of the ring kiln.
Once the leaf is fully laid, it is mortared over.
The mortar mix was soaked the previous evening.
Enough material for around eight minutes of work,
giving just the right quantity to coat both the inner and outer leaves.
The mortar seals out false air and keeps the heat in,
so particular attention is paid to the edges, which are pressed in firmly and smoothed off flat.
A second leaf is then built up roughly 60 centimetres in front of the first,
just one brick thick, 12 centimetres.
That outer leaf is mortared over as well.
The chamber doorway is now closed by two masonry leaves,
with an air gap between them, adding a useful layer of insulation.
Throughout all of this, loading blanks, closing doors, the kiln keeps burning without pause.
Blanks go into one chamber while finished bricks come out of the next.
The kiln master oversees the stacking, but he must keep one eye on the fire at all times.
The fuel here is brown coal dust and fines, lignite slack.
Current consumption runs at one and a half tonnes per day.
Every 30 minutes, the kiln master tops up the feed hoppers.
In earlier practice, every row of feed holes was charged by hand,
a method kept on today only for the residual fire section at Meckenheim.
The rearmost row of the automatic firing zone, visible here, is holding at 1,000 degrees.
Between the seventh and sixth rows lies the peak firing point,
where temperatures reach 1,080 degrees, while the leading row is still climbing toward 500 degrees.
Judging how the firing is going comes down to experience.
The bricks are done when a course is drawn in by five centimetres.
The feed hoppers are tripped automatically every 20 seconds.
The amount of fuel released depends on the adjustment.
At two notches, the charge is light.
At four notches, it is heavier, and the temperature climbs higher.
A strip chart recorder allows the kiln master to call up each of the four thermocouples per chamber in turn.
The trace shows a clear spike of around 20 degrees each time the hoppers discharge.
In the third row of the residual fire section, one such thermocouple is installed.
Here, the kiln master charges the hoppers by hand.
The first of the six rows is running at approximately 1,020 degrees, the last at around 900 degrees.
Two adjustable damper registers are open. The kiln is drawing well.
When a feed hole is lifted clear, the main fire flares up sharply,
confirmation that the kiln master has the draft dialed in correctly.
The firing has advanced far enough for the kiln master to move the last row of feed hoppers forward one step.
The automatic fire zone extends by one row, and the residual fire section follows behind it.
The hopper drive mechanism runs at three selectable speeds.
A pushrod linkage rises from the hoppers to a crank and chain assembly, just under the crown of the kiln roof.
A pin on the chain drives the rod back and forth, and from there the motion is carried across the full run of hoppers.
The mechanism alternates. On one cycle, it drives the outer and inner rows. On the next, the center row.
At the new position, the kiln master hooks the connecting link into the rotating drive ring,
then opens the feed hole beneath the hopper and sets it down in place.
Up to five rows of hoppers can be advanced in a day, depending on the rate of firing.
Today, with the burn running on the slow side, only three rows are moved forward.
This hopper now leads the automatic firing zone, where the temperature stands at roughly 500 degrees and should rise only gradually.
The kiln master sets it to the lightest feed, two notches.
While the kiln master moves hoppers forward, hand charges the residual fire, and monitors the burn,
stacking carries on in the chambers across the kiln.
On the far side of the residual fire section, the fired bricks are cooling.
The outer masonry leaf comes down first, then the inner one.
The bricks must not be opened to cold air too quickly, or they will crack.
The second gang works steadily through the chamber, clearing it out.
The still warm bricks are loaded onto a flat trolley.
Ring and color together tell the kiln master how well each brick has come through.
A deeply sunken frog is a sign the clay was too wet when pressed.
The bricks in the upper left of the stack carry a slightly elevated proportion of topsoil.
Bricks that meet the requirements of standard DIN 105, as common bricks are sold in packs of 200 to builders and private customers,
used mainly in exposed brickwork and for rustic interior work.
The Grafschafter kraut for brick puts them to use in every building job carried out on the factory site.
The finished courses lean slightly back in the chamber.
Around the feed holes, the ash and slag from combustion sit clearly on the brick surfaces.
The lignite slack has burned cleanly down to nothing.
Ring kilns were once a landmark in industrial progress.
Most have long since been replaced by tunnel kilns and other modern plant.
The Meckenheim ring kiln is now one of the last fully operational examples anywhere still in regular use.