Hello everyone, let us start lecture 7 and topic, we will now continue our discussion
on explanation corrosion processes on the basis of mixed potential theory.
When we in the last lecture at the end, we started talking on the evolution of microstructure
of pearlite and how it look, how it looks under the microscope, optical microscope.
This has a relation to the area ratio of a galvanic couple.
So, let us explain that particular microstructure.
So, it is actually a practical aspect of corrosion.
So, how to or explaining the typical microstructure of pearlite.
So, this is related to area of cathode and now in steel, the pearlite is a phase mixture
in a steel and that too we get it very low carbon steel, let us say 0.1 percent carbon,
we do not see the pearlite much, but as we increase the carbon content, let us say if
we go to 0.4 to 0.5 percent carbon, we can clearly notice pearlite and in the pearlite
the phase mixture, why call it phase mixture?
Because it consists of two phases, one is cementite and another one is ferrite.
So, ferrite is nothing but alpha iron which is a solid solution of carbon in BCC iron
and cementite Fe 3 C, this is a compound, this is a compound.
Now, their formation happens due to nucleation and growth phenomenon, so either ferrite or
cementite nucleates on a grain boundary and that too in the pre-austenitic grain boundary
and then gradually by the side of it, if cementite nucleates by the side of it ferrite nucleates
and then gradually this nucleation happens at the same time, side by nucleation keeps
on happening at the same time, you have the growth of the ferrite as well as cementite
into the austenite grain.
So, that means if we have a austenite grain boundary like this, so then if cementite nucleates,
this is a cementite let us say or I would say that Fe 3 C fine and then since cementite
takes carbon from the austenite, this is austenite, this is austenite, austenite it termed as
a gamma iron or austenite.
So, since carbon diffuses and then forms this Fe 3 C and the carbon in the Fe 3 C is 6.67
in terms of weight percent, so the surrounding area will be depleted in carbon and this particular
steel from the austenite, it has been taken to a region below eutectoid point.
So, that time by the side you will have a ferrite formation, this is ferrite, this is
ferrite.
So now, by the side then there will be a cementite nucleation again, cementite formation.
So, like that way at the same time, they keep growing along this direction fine.
So finally, your structure would be, so this is cementite, this is another cementite, this
is another cementite.
So, like this it forms a lamellar structure and this lamellar, so their growth may not
be absolutely a kind of a flat parallel lines, their actual look like this ok.
So, that time this is the look what we are getting in under the optical microscope.
Now, if we take a steel where let us say 0.4 percent carbon steel and that is annealed,
furnace annealed.
So, that means, I would say not furnace annealed, I would say the furnace cooled, so that means,
you take it to 900 degree Celsius, this particular carbon steel, then wait for some time let
us say half an hour, so that the complete austenite forms in that particular microstructure
and then you allow it to cool in the furnace by putting of the furnace.
So, that time you will have a slow cooling and once the temperature crosses below the
eutectoid temperature, which is around 727 degree Celsius and then you will have this
pearlitic reaction, this kind of structure evolves.
So, then you do this is the austenitization temperature for half an hour or let us say
45 minutes just to be on the safer side, so that every carbon goes into the solid solution
of gamma iron and then you cool it slowly furnace cooling.
So, you will have a structure like this, so you have austenite ferrite grain and then
you have pearlite, so like or this a kind of structure you will get, so where these
are the pearlite and these are alpha iron, alpha phase which is ferrite.
So, these are the ferrite which is have which has a special name called pro-eutectoid ferrite.
So, our interest is not on the detail of phase transformation, our interest is why
it looks like this, there is a black strips in the bright background.
Now, in order to understand this we need to understand little bit of etching and this
kind of steel is etched in around 3 percent nitrile solution and nitrile is a mixture
of nitric acid in alcohol.
So, these nitrile solution you first have the sample, you polish it go up to the mirror
polish, so that you can see your face reflected on that polish surface and then you hold it
with a tweezer, take this nitrile solution on a petri dish and then dip that particular
surface into the acid, wait for may be 2, 3 seconds or may be maximum 4, 5 seconds depending
on how much change you are facing, you are experiencing on the surface.
It will turn into little grayish or little darkish appearance that means the surface
is getting attacked by that particular solution and that particular process we call it etching
and this is nothing but etchant, we call it etchant.
So, now that chemical reaction we call it chemical reaction, but actually it is not
chemical reaction, it is electrochemical reaction and because of that particular electrochemical
nature of that reaction, we get to see appearance like this under under optical microscope.
So, now what exactly happens, so now you have those lamellas is not it, so you have ferrite,
you have cementite like this, those are aligned like this in a particular pearlite colony,
so these are cementite and these white portions are nothing but ferrite.
So, now when this surface is attacked, typically if we compare these two phases their electrochemical
behavior, this has higher potential in that galvanic series as compared to the ferrite.
So, this acts as a positive terminal and this acts as a negative terminal in that galvanic
couple condition.
So, they are actually forming a galvanic coupling, so once they form galvanic coupling since
this is negative that means this is anode and this becomes positive that means this
is cathode.
So, cathode would not dissolve, anode would start dissolving, but interesting part is
if we see this particular surface, this part is negative, this part is positive, so a dissolution
would follow the pattern what we have experienced before, so the experience we have experienced
like this that in the dissolution would be more pronounced near to the galvanic couple
region.
So, now if I consider here also the dissolution of ferrite will be more pronounced around
this region, this region, similarly here the dissolution would be more pronounced
around this region, away from that the dissolution of course it will dissolve, but the dissolution
rate would be slower because of the resistance offered by the electrolyte away from the galvanic
coupling or the point where the or the line where the galvanic coupling has been set up.
So, now if they dissolve like this, if we put it in a red color, so now their dissolution
pattern would be like this fine, so that means you see that this is the surface line, so
everywhere that dissolution has taken place, but the dissolution is more pronounced around
this segment, this segment.
Now if we see, if we zoom one particular region, one particular region, this is the
cementite, this is the cementite, now here we have situation like this at depth, now
how do we see the structure in optical microscope?
We see it because the light which is falling, so you have a surface, the lights are falling,
lights are falling and then they are getting reflected and you have an eyepiece, eyepiece,
so this eyepiece you look at and then see the structure, so basically it is a magic
of reflection of light in the optical microscope.
So, now when you have a situation, if it is a flat surface, if it is a flat surface before
etching, it is a flat surface and it shines, why it shines?
Because all the points over which those reflections are taking place of the light are happening
at the same condition and the energy of the light which is coming out are almost of the
similar range, so that is what there is no multiple reflection within a small region,
if we consider the small region, not much of multiple reflections are taking place within
that particular region, so that is what we are having appearance of a very shiny surface.
But if I consider a situation like this, so here the lights are falling, here also lights
are falling, so they are reflected, they are reflected and since it is a almost a kind
of a flat region, a near flat region, so the surface look, these surfaces from this
particular zone, this surfaces at this section, at this section they look shiny or the bright.
But if I consider here in this zone, what happens?
Let us say one light has fallen like this, now here we have to consider a reflection
angle, now it will go like this fine and when it goes like this, that could be hindered
by this cementite plate thickness or if that reflection, because if we consider the cross
section, the cross section look as a circular region, on the centre we have cementite.
So if it is falling away from that particular, if it reflecting away from that particular
cementite rod, rod like or plate like appearance, so then it will have a reflection here, multiple
reflection will and then again you will have a angle like this, it will go like this.
So it is not coming back to the eyepiece, here we have eyepiece fine.
Similarly if another light falls like this, so you have a angle like this, it might go
like this fine.
So like that there could be a multiple, a kind of reflection that will take place, so
those reflection might not come back to the eyepiece.
So if they do not come back to the eyepiece, so that means the energy that is being taken
by those rays, I would say that the number of rays coming out from those regions, these
particular region will be less than the lights coming out from this flat regions.
So what would happen?
It would look like a dark region.
So if something looking dark, within that it is small a pin kind of thing or the plate
kind of thing that would look like a dark object ok.
So that is why we see this particular cementite to be dark and interestingly this darkness
comes because of multiple reflection and those lights will not come out to the and it will
not go to the eyepiece.
So it will look dark and this region will look bright.
So this region will look dark and this region will look bright.
So if we consider here, this section, this section, so this section, this section they
will dark, they will be dark and this regions will be.
So the and interestingly these are the regions or the dimension is hardly a few microns may
be around 10 to 20 microns.
So that time, so if this is that much dimension, so then what happens?
In the optical microscope the resolution is less, so it will not be able to gauge the
position of that cementite properly.
it will show a kind of dark patch around that.
So that for the final microstructure would look like this where this is alpha or ferrite
and this is cementite.
So this, so why we have explained this because it has a relation with the area and the resistance
effect during electrochemical etching process and this relates to the understanding what
we had in our previous lecture is this.
So let us go to understanding of those five instances, the situations, five situations
we had what we have talked about.
Now first instance is situation or instance of situation is here we have one cathodic
reaction plus one anodic reaction.
So in this case we have already explained this before while we consider corrosion of
zinc in deaerated pure HCL.
So that case our mixed potential theory was, so this is E, this is log I and the plot look
like this.
So this is I0 for the zinc over zinc surface.
This is I0 of hydrogen over zinc surface.
This is Ia of hydrogen.
So that means H2 – 2e equal to 2H+, this reaction would happen and this line corresponds
to Ic H2 2e equal to H2.
This line corresponds to Ia zinc which is nothing but zinc minus 2e equal to zinc plus
plus and this line is Ic zinc which is plus plus plus 2e equal to zinc and this is the
point which is E mix which is nothing but E corr and this point is I corr and this
current density meets the basic of mixed potential theory where it is Ic equal to Ia is nothing
but Ic hydrogen over zinc surface equal to Ic zinc Ia zinc.
So that means this is the complete picture of that particular mixed potential theory
for explaining this particular situation.
We have already explained it in detail I think end of fifth lecture.
So the overall reaction is overall electrochemical reaction is zinc plus HCl equal to zinc chloride
plus H2 where this is plus, this is 0, this is plus plus, this is minus, this is minus,
this is 0.
So we have oxidation.
We have reduction.
So let us go to the situation where we have considered two cathodic reaction and one
anodic reaction.
Now this particular thing can be explained can be observed when we see zinc corrosion
in deaerated HCl with some impurity in the form of Fe plus 3 iron.
Now deaerated means thus that HCl does not have any dissolve oxygen and that particular
so interestingly so if you leave HCl in the atmosphere it will always have some dissolve
oxygen.
Now how do we take care of that oxygen or how do we take out those oxygen dissolve oxygen
from the HCl.
So what in the lab scale what is done is we purge nitrogen into the solution.
So the nitrogen bubbling happens and that releases dissolve oxygen out of the HCl solution.
So this impurity Fe plus 3 is a small impurity a very small amount some ppm level what would
happen.
Now in this case let us first analyze what are those two cathodic reaction and one anodic
reaction.
So the anodic reaction it is easy to understand.
It is zinc minus 2e equal to zinc plus plus this is anodic one anodic.
Now what are the cathodic reactions?
Of course if it is an acid solution so the cathodic reaction of course this is the cathodic
reaction and we would we do see that hydrogen bubbling is taking place on the zinc.
Now interestingly just before going into this explanation the observation that has been
observation is typical observation is if you consider this particular case here also hydrogen
bubbling takes place on the zinc surface and here also hydrogen bubbling takes place on
the zinc surface and we do get zinc corrosion.
Now the hydrogen bubbling amount or I would say that the bubble formed across the surface
would be much less in this case as compared to this case.
So we would also understand that particular observation through mixed potential theory.
Now this is cathodic reaction.
Now where is the another cathodic reaction?
Another cathodic reaction happens in this form.
So this is also cathodic reaction and interestingly this is a very, very strong cathodic reaction.
Why?
So if we consider standard reduction potential E0 this one is 0.76 minus volt, this one
is 0 volt and this one is plus 0.77 volt and that to all at 25 degree Celsius and one
atmosphere pressure.
So that condition these are the potential the standard reduction potential.
So now we can see that the difference between this two is huge.
So that means and also even if we consider these two the difference is huge.
So that means this is a much stronger cathodic reaction than this.
So now we could see that there are two cathodic reactions and one anodic reactions and overall
process of course zinc would dissolve and these two cathodic reactions would happen
on the surface of the zinc.
So we would analyze this particular situation in our next lecture.
So let us stop here.
Thank you.