So, welcome again to the new lecture, this is lecture number 26 of phase equilibrium
course. So, we will first recap the contents of the last lecture. So, in the last lecture
we looked at how to calculate the phase fractions in a binary eutectic system, especially concentrating
at hyper eutectic composition. So, we correlated the components of different phases and then
we looked at few example phase diagrams. So, we looked at copper nickel which was a isomorphous
system. So, we looked at how the microstructure of a copper nickel system looks, it does not
look like a perfectly homogeneous system, it looks like a micro graph showing some contrast
which is basically due to composition contrast. And then we looked at aluminum silicon system
which makes a eutectic system. So, this is isomorphous and this is eutectic which although
it makes a eutectic system, there is very little solid solubility at lower temperatures.
And as a result the mixture is basically aluminum and silicon, then silicon being present in
morphology which is deleterious to mechanical properties. As a result grain refiners, the
refiners always are microstructural refiners are added to improve the morphology of silicon
to have to. So, that alloy can have better mechanical properties. In this lecture we
will look at some more alloy systems of commercial importance and see what kind of reactions
they possess and what kind of microstructures that we obtain in those systems.
So, the examples that we will look at in this first example is lead tin system which is
a eutectic system. So, let us see how it looks like. So, this is lead tin phase diagram,
it is a binary eutectic phase diagram with considerable solid solubility at eutectic
temperature. So, lead is FCC, tin is has a different crystal structure which has different
crystal structure as compared to tin. They make two solid solutions alpha and beta for
lead rich and tin rich ends. Lead rich side has considerable solid solubility at eutectic
temperature about 18.3 percent whereas, the solid solubility of tin lead and tin is very
little it is about 4 to 5 percent as a result it makes a beta phase which has very little
solid solubility at lower temperature, but reasonable solid solubility at high temperature.
They have a eutectic mixture at 61.9 percent tin which eutectic mixture converts directly
into unferred beta phases and they have this terminal solid solubilities of 18.3 percent
at high temperature of. So, eutectic temperature is 183 degree centigrade at eutectic temperatures
the solid solubility is 18.3 percent this is I think about 95 percent let me see. So,
the region which is between this 18.3 and 61.9 is called as hyper eutectic region whereas,
the region between 61.9 and let me it is about I think it is about 96 percent roughly
I may be wrong, but it is about it is in this range. So, between this 61.9 and this point
the alloy is called as hyper eutectic. So, of course, so we will we will show you
how three. So, microstructures look like. So, we will look at microstructures in the
three. So, we will look at microstructure which is of hyper eutectic, eutectic and hyper
eutectic. So, these are the three compositions. So, hyper eutectic alloys of composition 50
weight percent tin, eutectic composition is of 61.9 percent tin and hyper eutectic basically
is of high composition roughly perhaps about 80 percent or 90 percent tin.
What we have here is we have in the hyper eutectic phase diagram you can in the microstructure
you can see that if you draw a line somewhere here 50 percent is this line. So, you can
see that you have pro eutectic pro eutectic alpha present at this point. So, what we have
is let me just change again color with the green one. So, at this point we have pro eutectic
alpha and at this point this pro eutectic alpha and liquid must have been there liquid
of this composition this liquid transforms into mixture of alpha and beta. So, what you
have this lamellar structure where you can see this parallel white and black plates at
various places this is all eutectic. So, this is eutectic mixture of alpha and beta present
along with hypo eutectic alpha. So, you can find out the proportions in the manner I explained
earlier. So, you can see that this alpha phases of the. So, this is 175 micron. So, you can
see that this alpha phase is nearly you know about 20, 30 microns. So, whereas, the size
of constituents in the eutectic is far smaller which is basically because eutectic converts
into solid all of a sudden as a result phases do not have too much time to grow and since
phases do not have too much time to grow the phases are finer as compared to the pro eutectic
phase. So, alpha and beta sizes are lower smaller as compared to pro eutectic phases
in the hypo hyper eutectic phase. Similarly, if you look at hyper eutectic region you have
pro eutectic beta along with eutectic phase. So, this is the eutectic phase again you can
see that the size of beta phase is smaller as compared to pro eutectic phase. So, hypo
and hyper eutectic microstructures are fairly similar except that the pro eutectic phases
are alpha in one case and beta in another case whereas, in the eutectic phase the image
for this composition. So, this is for hypo eutectic alloy for eutectic composition you
have only 6 eutectic phase. So, what you have is only the parallel plates of alpha and beta.
So, what you have this is. So, you can say that this black one is alpha and the grey
one is beta and these alpha and beta grows together and they form these colonies. So,
essentially if you look at microscopically alpha and beta grow in this fashion. So, let
us say one of them is. So, let us say this is alpha and the other one is beta and remember
alpha is lead rich which means it has to reject tin, beta is tin rich it has to reject lead.
So, partitioning of solute has to happen which means tin needs to travel this side and lead
needs to travel this side as a result simultaneous growth and simultaneous solute partitioning
has to happen there is not enough time for this to happen as a result the eutectic is
generally finer mixture as compared to pro eutectic alpha or beta. So, this is the microstructure
that you are likely to observe in case of a eutectic mixture of lead and tin.
Now, let us come to next important alloy which is of commercial importance which is. So,
the next one is iron carbon system and this is a complex phase diagram it has peritectic
it has eutectic and it has eutectoid reactions. So, this is how. So, again this is the zoomed
up image of microstructure of eutectic composition. So, the eutectic shows the parallel lamellas
of alpha and beta whereas, this is the hypoeutectic alloy 50 percent tin 50 percent lead. So,
you can see that alpha which is alpha phase which is the lead rich phase is proeutectic
phase and then you have a mixture of alpha and beta as eutectic.
Now, this is the celebrated iron carbon diagram. Now, this is generally iron carbon diagram
is from 0 percent carbon to 6.7 weight percent carbon basically 6.67 weight percent carbon
means F e 3 C. So, essentially it is F e 3 C phase diagram and F e 3 C consists of consists
of 6.7 percent carbon in weight wise. So, it is from 0 to 6.7 percent carbon region
phase diagram. So, what this phase diagram has is it has multiple regions you know carbon
is carbon has different structure different atomic radius as compared to iron as a result
they may they do not have complete solubility in various forms carbon and iron also react
to form intermetallic compound called as F e 3 C at. So, if you have 6.7 weight percent
carbon it will make F e 3 C compound. So, everything will be 100 percent F e 3 C what
it has is it has 3 regions the first region is this peritectic region which is that carbon
compositions lower than 0.5 percent then we have at. So, this is at 1493 degree centigrade
then we have another region at 1147 degree centigrade in the vicinity of this temperature
starting from 2.1 percent to 6.7 percent we have this region called as eutectic region.
And then at lower temperatures at 727 degree centigrade the phase of the gamma phase of
iron transforms into alpha plus cementite which is F e 3 C at a composition of 0.676.
So, we have this as a eutectoid region. So, there are 3 regions of the phase diagram the
peritectic region, the eutectic region and the eutectoid region and these are 3 invariate
reactions that occur in iron carbon phase diagram. So, let us look at each of these
regions. So, we first look at the region which is the peritectic region. So, in the what
we did was we first looked at lead tin alloy and now we are looking at iron carbon alloy
phase. So, iron carbon the first region is the peritectic
region peritectic region. So, if I just draw that particular line it has. So, basically
what happens is that here you have liquid present here this is at 1493 degree centigrade
97 or 93 let me check it is 1493 degree centigrade. So, this is temperature axis this is 0.1 percent
this is 0.15 percent and this is 0.5 percent carbon. So, in this at high temperatures for
pure carbon you have this delta phase delta phase of carbon which has B C C structure
if you increase the temperature if you increase the iron content further this delta phase
coexist with the liquid phase and you can draw the composition of 2 phases you can determine
the composition using tie line. This delta phase and liquid phase delta phase
of composition 0.1 percent and liquid phase of composition 0.5 percent transform into
gamma phase which is F C C phase of composition 0.15 percent through a peritectic reaction.
So, liquid plus delta transforming into gamma liquid of composition 0.5 delta of composition
0.1 and gamma of composition 0.15. So, in a peritectic reaction the solid which forms
has a composition intermediate to liquid and solid temperature and the liquid solid liquid
composition is on 1 extreme this is the identification of peritectic reaction. So, this and this
region is basically liquid plus. So, this is the peritectic region of the phase diagram
and you can see the you can draw the micro structural development the way it happened
in. So, this is delta plus gamma region and this is liquid plus if you look at the right
part of the phase diagram which is a eutectic part in the eutectic part you can see that
we have liquid transforming into a mixture of gamma phase plus cementite at a composition
of 4.3 percent and at a temperature of 1147 degree centigrade.
So, if I draw this eutectic region. So, this is the composition 4.3 percent this is 6.7
and somewhere here you have 2.1 percent. So, you have this is 1147 degree centigrade
and of course, you have and this these 2 lines coming from top from the peritectic region.
So, you have liquid plus gamma liquid plus Fe 3 C which is cementite and these 2 this
converts into gamma plus Fe 3 C at this temperature. So, this is the eutectic reaction. So, liquid
of composition 4.3 percent transforms into gamma of composition 2.1 percent plus Fe 3
C which is 6.7 percent carbon basically. Now, here the difference between alpha delta
delta and gamma is delta is solid solution of carbon and iron at high temperature and
its solid solubility varies up to the limit of solid solubility. Similarly, gamma is it
has a BCC structure. Similarly, you have gamma iron which is again solid solution
and it has a FCC structure whereas, Fe 3 C is called as cementite it is not a solid solution
it is a line compound or you can say it is a inter metallic it is much stronger than
alpha and delta iron it is very hard. So, comparatively gamma and delta delta and
gamma are very soft phases Fe 3 C is extremely hard very hard. Now, the third part of iron
carbon phase diagram is the eutectoid part and this is the most important phase diagram
this is most important part of the phase diagram as far as engineering applications of iron
phase diagram are concerned. In this part of the phase diagram the gamma phase of composition
0.76 percent which is solid phase transforms into a mixture of alpha iron which has very
low solid solubility of carbon in iron about 0.022 percent plus cementite. So, what it
does is basically. So, it has you have a like this. So, this is a temperature 727 degree
centigrade. So, this is point nearly 0.8 percent this is 0.02 percent and this goes all the
way the interesting part of phase diagram is only up to 2 percent. So, gamma iron which
is F C C converts into alpha plus Fe 3 C and this is pure alpha this is alpha plus gamma
this is gamma plus Fe 3 C. So, the region which is left of 0.8 percent
is called as hypo eutectoid. So, less than 0.8 percent the region which is right of 0.8
percent is called as hyper eutectoid and iron with carbon less than 2 percent less than
or equal to 2 percent is called as steel. This is these compositions make up the modern
material called as a steel and this is it is it is the it is this part of the phase
diagram of iron carbon which is extremely interesting for from the perspective of engineering
this material for variety of applications. So, what you have here is you have single
phase gamma which is F C C structure. So, when you start in this region you have these
grains of gamma. So, this is gamma all now depending upon whether you are cooling now
depending upon whether you are cooling from this point whether you are in this point whether
you are in this region you will obtain different microstructure. So, you can see that the microstructure
is going to be fairly similar to what you obtain in eutectic it is just that it is going
to happen in solid state and since it happens in solid state the feature size is even smaller
because the diffusion distances are smaller in solid phase.
So, what you have here is you have this composition 0.8 percent composition which is called as
eutectoid steel then we have less than 0.8 percent which is called as hypo eutectoid
steel and then we have steel between 0.8 percent and 2 percent is called as hyper eutectoid
steel and it is the three phase three kinds of phase distributions which are important
from the perspective of engineering applications of this alloy. So, and anything beyond 4 percent
beyond 2 percent carbon is called as cast iron. So, if you if you if your carbon content
is between 2 percent to 6.7 percent alloy will be called as cast iron if your composition
of the alloy is below 0.8 percent 0.76 percent to be precise it is called as hypo eutectoid
steel and if it is between 0.76 to 2 percent carbon it is called as hyper eutectoid steel.
So, this region is steel and this region is cast iron and there are various phases liquid
phase is present at high temperature delta Fe which is a polymorph of allotrope of iron
is present at high temperature for very low percentages of carbon or for pure carbon gamma
phase which is the FCC structured phase called as austenite this phase is present from this
has maximum solid solubility of 2 percent 2.1 percent at a temperature of 1147 degree
centigrade and it has very large single phase region starting from peritectic temperature
of 1493 degree centigrade to the eutectoid temperature of 727 degree centigrade. So,
this whole region is single phase gamma region FCC structure, but this is unstable phase
because the high temperature phase this transforms into two phases at lower temperature one is
called as alpha Fe which is which is called as ferrite alpha Fe is called as ferrite it
has very little solid solubility of carbon in iron it is a soft phase of iron and second
phase which forms at low temperature is called as cementite which is Fe 3 C cementite.
And it is the microstructure of these three regions which is of importance. So, microstructure
of this region microstructure at this point and microstructure at this point which is
what is important from the perspective of engineering applications and these microstructures
can be tailored modified quite extensively by adopting different cooling rates etcetera.
So, there are three invariant reactions that happen at 1493 degree centigrade peritectic
reaction occurs liquid of composition 0.5 percent delta of and delta iron of composition
0.1 percent transform together to give gamma iron of composition 0.16 percent this is 0.16
percent. 1147 degree centigrade you have eutectic reaction in which liquid of composition 4.2
percent transforms to gamma iron of 2.1 percent and Fe 3 C a line compound at 727 degree centigrade
eutectoid reaction occurs at which in which gamma iron of composition 0.8 percent transforms
into alpha iron of 0.002 percent solid solubility and Fe 3 C these are three major invariant
reactions that occur in iron carbon phase diagram.
Now, let us look at what are the what are the microstructures that we obtain if you
have 0.8 weight percent carbon steel which is 0.7 basically 0.76 eutectoid we call it
eutectoid steel the composition for which the gamma phase. So, eutectoid steel is the
one. So, eutectoid steel is the one for which carbon content is in the vicinity of 0.8 percent.
So, basically in this the gamma phase converts into a mixture of alpha Fe which has a solid
solubility of 0.02 percent plus Fe 3 C and this is a eutectoid mixture it forms all of
a sudden. So, you had started with grains of gamma this is all gamma and then you suddenly
convert this into a mixture. So, you had these grain boundaries of gamma on these grain
boundaries of gamma you have nucleation and growth of. So, this is how they will form.
So, these colonies will form. So, this is a alpha Fe plus Fe 3 C colony this is called
as lamellar structure lamellar structure of and if you look at it microscopically what
it is going to look like it is going to look like this you have plate of let me use a different
color here. So, you have a plate of alpha then you have. So, these are the plates of
alpha. So, you have alpha in between you have Fe 3 C and again just like eutectic you are
going to have partitioning of solute. So, alpha will release carbon which will get into
Fe 3 C and iron will transform iron will move from other side to make alpha Fe. So, this
is Fe rich and this is carbon rich. So, that is why they form a parallel lamellar structure
and what you see in the micro graph is something like this. So, you see sort of grayish micro
structure in which you can see these are the parallel plates. So, you have this as a parallel
plate you can see these are the parallel plates. So, you can see and if you zoom it
up in the microstructure these are the parallel plates. So, you have plates of cementite parallel
to ferrite. So, this is how the microstructure looks like if you want a final description
of the microstructure let us look at the next. So, this is the final description of the microstructure
you have these parallel plates of alpha and Fe. So, alpha is the brighter phase you can
see that there is larger proportion of alpha than cementite. So, thicker plates will be
that of ferrite and the thinner plate will be of that of cementite you can see this kind
of parallel plate microstructure lamellar microstructure that you will see and this
is called as pearlitic microstructure the pearlite is not a phase it is just a mixture
of alpha Fe and cementite. So, in steel this mixture of eutectic mixture
of alpha Fe plus Fe 3 C is called as pearlite. So, as long as you have a microstructure which
has this kind of morphology which is lamellar morphology the microstructure will be called
as a pearlitic microstructure and the microstructure of other two sides will be very different
which we will look at in the next lecture. So, what we have done in that in this lecture
is we have again looked at a few common phase diagrams such as lead tin phase diagram and
iron carbon phase diagram we have looked at the various invariant reactions in the
iron phase carbon phase diagram and also how the microstructure looks for a eutectoid steel
in the next lecture we will further develop on it we will look at the microstructures
of hypo and hyper eutectoid steels as well as a few cast irons before we move on to the
next part of the course.